Aliaje fuzibile
Aliajele fuzibile sunt aliaje cu puncte de topire la temperaturi ambientale. Un exemlu ar fi cele bazate pe galiu.
Exemple
Aliaje fusibile la temperaturi joase
Compoziție - procent masic
|
°C
|
eutectic?
|
Nume sau remarcă
|
Cs 73.71, K 22.14, Na 4.14[1] |
−78.2 |
da
|
Hg 91.5, Tl 8.5 |
−58 |
yes |
folosit in termometre de temperaturi joase
|
Hg 100 |
−38.8 |
(da)
|
Cs 77.0, K 23.0 |
−37.5 |
|
K 76.7, Na 23.3 |
−12.7 |
da
|
K 78.0, Na 22.0 |
−11 |
nu |
NaK
|
Ga 61 , In 25, Sn 13, Zn 1 |
8.5 |
da
|
Ga 62.5, In 21.5, Sn 16.0 |
10.7 |
da
|
Ga 69.8, In 17.6, Sn 12.5 |
10.8 |
nu
|
Ga 68.5, In 21.5, Sn 10 |
11 |
no |
Galinstan
|
Ga 75.5, In 24.5 |
15.7 |
da
|
Cs 100 |
28.6 |
da
|
Ga 100 |
29.8 |
da
|
Bi 40.3, Pb 22.2, In 17.2, Sn 10.7, Cd 8.1, Tl 1.1 |
41.5 |
da
|
Bi 40.63, Pb 22.1, In 18.1, Sn 10.65, Cd 8.2 |
46.5 |
|
Bi 32.5, In 51.0, Sn 16.5 |
60.5 |
yes |
metalul lui Field
|
Bi 49.5, Pb 27.3, Sn 13.1, Cd 10.1 |
70.9 |
yes |
aliaj Lipowitz
|
Bi 50.0, Pb 25.0, Sn 12.5, Cd 12.5 |
71 |
no |
metal Wood
|
In 66.3, Bi 33.7 |
72 |
da
|
Bi 52.5, Pb 32.0, Sn 15.5 |
95 |
da
|
Bi 50.0, Pb 31.2, Sn 18.8 |
97 |
nu |
metalul lui Newton
|
Bi 50.0, Pb 28.0, Sn 22.0 |
109 |
nu |
metalul lui Rose
|
Bi 56.5, Pb 43.5 |
125 |
da
|
Bi 58 , Sn 42 |
139 |
da
|
In 100 |
157 |
da
|
Sn 62.3, Pb 37.7 |
183 |
da
|
Sn 63.0, Pb 37.0 |
183 |
nu |
Eutectic solder
|
Sn 91.0, Zn 9.0 |
198 |
da
|
Sn 92.0, Zn 8.0 |
199 |
nu |
staniu folie
|
Note
- ^ Oshe, Ed. R.W., "Handbook of Thermodynamic and Transport Properties of Alkali Metals", Oxford. UK, Blackwell Scientific Publications Ltd, 1985, p. 987
Vezi și
Legături externe
|
|